Samples mill annealed and cold worked yielded the following room temperature tensile results:
Cold Work |
Yield Strength |
Ultimate Tensile Strength |
Elongation |
% |
ksi |
MPa |
ksi |
MPa |
% |
0 |
74 |
510 |
134 |
924 |
57 |
10 |
112 |
772 |
150 |
1034 |
38 |
20 |
142 |
979 |
167 |
1151 |
26 |
30 |
168 |
1158 |
191 |
1317 |
14 |
40 |
194 |
1338 |
215 |
1482 |
8 |